News
The Thread That Passed And Would Not Start
The complaint came from assembly rather than from quality: a batch of housings had passed visual inspection with the threads marked complete, and a third of them would not accept a bolt by hand. Some started and seized; some refused at the first turn.
Thread inspection is the check that looks simplest on a control plan and is one of the harder ones to do with a camera, because a thread is not a shape you can see; it is a surface that has been cut into a spiral, and the part of it that matters is often facing away from the lens.
Day One: What The Images Showed
The first thing checked was whether the station had flagged anything at all in that batch. It had not. Every thread in the sample had been imaged, judged, and stored.
The stored images were then reviewed against the criterion in the control plan, which said the thread form must be complete and free of damage. On the images, it was. The crests were continuous, no visible tearing, no missing turns.
So either the parts were good and assembly was wrong, or the criterion was describing something different from what assembly needed. The second was true, and it took a sectioned part to show it.
Day Two: What The Section Showed
Two housings were cut through a threaded bore and examined. One had passed and would accept a bolt; one had passed and would not.
The difference was at the root of the thread, not at the crest. On the failing part, a thin ridge of material sat along the root, left by the tapping tool and never removed. It was under 0.3 mm high and it did not touch the crest line, so from the direction the camera was looking it was invisible: the crest was complete, and the root was behind the crest.
That is the geometry of the problem. A camera looking into a threaded bore sees the crest of each turn and, at best, a sliver of the flank. The root is occluded by the crest in front of it. A ridge in the root is a real defect and a real assembly problem, and it is hidden by the feature that the inspection was designed around.
Day Three: Why The Criterion Did Not Catch It
The criterion said the thread form must be complete, which is a statement about the crest. Nobody had written down what degree of root cleanliness was required, because the root had never been considered.
This is common in thread inspection: the visible failure modes are missing threads, damaged crests and cross-threading, and all three are visible from the front. The failure modes that cause assembly problems are root burrs, chips lodged in the flank, and partial threads at the start of the bore, and none of those are visible from the front.
The station was doing exactly what it was asked. The specification had described the easy half of the defect population.
What Changed
Four things, in order of effect.
The tapping process was changed to reduce root burrs at source, which is the only real fix and the one that costs the least in the long run. Deburring after tapping was reviewed, because a brush that cleans the crest does not reach the root.
The thread inspection criterion was rewritten around what assembly needs: not thread form complete, but no material in the root exceeding a stated height, and no obstruction in the first two turns. That second clause matters because a bolt that will not start is a bolt that meets an obstruction at the entrance, whatever the rest of the thread looks like.
The imaging was changed from a single axial view to two oblique views, which exposes part of the flank and makes a root ridge cast a shadow rather than hide behind a crest. It is not a full view of the root; it is enough to catch a ridge above the threshold.
And a go/no-go gauge was introduced as a sample check on every shift, because the only definitive test of whether a thread accepts a bolt is a bolt.
Where Thread Inspection Actually Stands
External threads are easier: the flank and the root are both accessible, and a low-angle light makes a root burr obvious. Internal threads are the hard case, and the smaller the bore the harder, because the crest occludes a larger fraction of the root as the diameter falls.
The requirement that appears in serious specifications is thread form integrity including internal bores, which is a statement that the hard case is in scope. Delivering it takes oblique or rotary imaging and a criterion written in terms of the root rather than the crest, and it takes a gauge as the reference, because no image is a substitute for a bolt entering.
What I Still Do Not Know
I cannot tell you the root burr height at which a bolt starts to bind, because it depends on the bolt, the pitch and the engagement length, and I have only one case.
What I can say is that a thread inspection criterion written around visible completeness will pass parts that assembly rejects, and that the gap between the two is at the root. Any specification for thread inspection should be able to answer one question: what does the check do about the surface the camera cannot see?